This is our QC acceptance standard. We check every part against it before it ships, and we use it to decide every defect report.
| Document |
QC acceptance standard |
| Revision |
1.0 |
| Effective |
November 19, 2026 |
| Applies to |
All orders except At Risk orders |
| Reporting window |
10 calendar days from delivery |
1. Acceptance criteria
A part in the "Fails QC" column is a defect, and we fix it at no charge. Results in the "Passes QC" column are normal.
| Check |
Fails QC (defect) |
Passes QC (normal) |
| Part, material, color, quantity |
Does not match the order |
Matches the order |
| Dimensions |
Overall length, width or height outside the tolerance in table 3 |
Within the tolerance in table 3 |
| Flatness |
Warped, bowed or lifted at the corners beyond the tolerance in table 3 |
Within the tolerance in table 3 |
| Structural integrity |
Layers separating (delamination), cracks, or a missing feature that is in the file and at or above the minimum wall |
A feature below the minimum wall that prints weak, flexes or breaks |
| Holes and channels |
A hole, slot or channel that is open in the file and at or above the min hole in table 3 comes out closed, blocked, or with resin or powder left in it |
A hole, slot or channel below the min hole that closes up or keeps some resin or powder |
| Resin cure |
Tacky, wet or soft to the touch at delivery |
A dry surface. Thin sections flex even when fully cured. |
| Ordered finish |
A finish on the order is missing or done wrong |
The finish on the order is done |
2. Surface finish
| Check |
Fails QC (defect) |
Passes QC (normal) |
| Layer lines |
A step or offset where the layers shifted |
Even layer lines for the technology and quality level ordered |
| Support removal |
Supports or support residue left on, or gouges from removing them |
Small nubs or sanded spots where supports touched |
| Blemishes |
Blobs, pits, holes or scratches that are not part of the normal surface in table 4 |
The normal surface in table 4 |
| Stringing (FDM, FGF) |
Strings or fine hairs left on the part |
No strings left after cleanup |
| Extrusion (FDM, FGF) |
Gaps between lines, or bulging, rough walls |
Continuous, even walls |
| Powder (MJF) |
Loose powder left on the outside of the part |
A clean, slightly grainy surface |
| Color |
A different color from the order |
Small shade differences between print batches |
| Paint we applied |
Drips, runs, bare spots or trapped dust |
An even coat. Layer lines can show under paint unless sanding was ordered. |
3. Tolerances and minimum sizes
| Technology |
Tolerance |
Min wall |
Min hole |
| FDM |
±0.5 mm or ±0.5% |
1.0 mm |
2.0 mm |
| SLA |
±0.2 mm or ±0.2% |
1.0 mm |
2.0 mm |
| Industrial SLA |
±0.2 mm or ±0.2% |
1.0 mm |
2.0 mm |
| MJF |
±0.3 mm or ±0.3% |
1.0 mm |
1.5 mm |
| FGF |
±1.0 mm or ±0.5% |
4.5 mm |
3.0 mm |
Tolerance is whichever of the two values is greater. Min hole is the smallest hole, slot or channel that comes out open and clear of resin or powder. We measure it on the part's overall length, width and height with calibrated calipers. Example: a 300 mm FDM part is within tolerance at ±1.5 mm. If a smaller feature is critical, tell us when you order and we'll confirm whether we can hold it.
4. Normal surface and defects by technology
| Technology |
Normal surface (passes) |
Defects (fails) |
| FDM |
Visible layer lines on sides and curves, a small seam line where each layer starts, a slight texture on the face that sat on the bed, rougher faces where supports touched |
Layer shift, stringing, gaps or bulging walls, warped or lifted corners beyond tolerance, layers splitting |
| SLA |
Smooth with very fine layer lines, small nubs or sanded spots at support points, a slight yellow tint over time |
Layers separating, holes or craters, cracks, a tacky surface, supports left on |
| Industrial SLA |
Same as SLA, at a larger size |
Same as SLA |
| MJF |
Even, matte, slightly grainy and porous surface, gray in its natural color, no support marks |
Loose powder left on the outside, warping beyond tolerance, cracks |
| FGF |
Clearly visible thick layer lines from a larger nozzle, a seam line, a rougher overall surface |
Layer shift, layers splitting, gaps or bulging walls, warping beyond tolerance |
5. Not defects
| Condition |
Why |
| Breakage or damage after delivery, during handling, assembly or use |
It happens after the part passed QC |
| Painting, solvents or other finishing done elsewhere |
It is outside our process |
| Resin yellowing or becoming more brittle in sunlight or UV light |
Normal aging of resin |
| Issues we warned you about on an At Risk order |
You approved the risk before printing |
| Damage in shipping |
Covered separately: What should I do if my part arrives damaged? |
6. Reporting a defect
| Item |
Requirement |
| Window |
10 calendar days from delivery |
| Where |
The support chat on this page |
| Include |
Your order number and clear photos of the problem |
| Return the part |
Not needed |
| How we decide |
We compare your photos with the photos we took before shipping |
| What happens next |
Reprint policy and refund policy |
Makelab is a professional 3D printing service in Brooklyn, NYC offering on-demand FDM, SLA, Industrial SLA, MJF, and FGF 3D printing. We serve designers, engineers, and businesses with custom 3D printing services — from rapid prototyping to production parts. Get an instant quote or chat with our team.